# Catalogue of damping materials

> One page of the phonometry documentation, as Markdown. Index: https://docs.jmrp.io/phonometry/llms.txt

Canonical: https://docs.jmrp.io/phonometry/reference/catalogues/damping-materials/
Language: en
Alternate: https://docs.jmrp.io/phonometry/es/reference/catalogues/damping-materials/index.md
Version: phonometry 4.0.0
Install: pip install "phonometry[full]"
Author: José Manuel Requena Plens (https://orcid.org/0000-0003-1250-6212)
Published: 2026-10-28
Updated: 2026-11-16T21:36:14Z
Summary: Seventeen commercial damping materials: the peak loss factor, the temperature of the peak at 10 Hz, 100 Hz and 1 kHz, and the storage and loss moduli.

---

Seventeen commercial damping treatments, and one thing about them that makes
this a different table from the [solids
catalogue](https://docs.jmrp.io/phonometry/reference/catalogues/solids/): a loss factor here is not
a number. Every loss factor in the solids catalogue is a single figure, because
for a metal it hardly moves. For a polymer worked near its glass transition it
moves by two orders of magnitude with temperature and with frequency, and the
peak is all these pages print. So the peak arrives with three temperatures
beside it, one per frequency the table prints a column for: where the material
peaks when it is worked at 10 Hz, at 100 Hz and at 1 kHz. A treatment whose
peak sits at 20 °C at 100 Hz is doing nothing for you at 100 Hz on a winter
morning, and a row read without its temperatures says the opposite of what it
holds.

The three storage moduli are the same argument again. One is the stiff end, at
low temperature or high frequency, one is the soft end, and one is the modulus
that applies in the band where the loss factor peaks, which is the only one of
the three that belongs beside the peak. The fourth column is the loss modulus,
the imaginary part, which the chapter gives as the product of the other two and
is the cheapest check there is on a row. The page is in degrees Fahrenheit and
pounds per square inch, so every temperature and every modulus here was
converted and is marked as converted, with the page's figure and its unit
beside it. The loss factor is the one column that was not: it has
no units, so it is served exactly as printed. The page says in a footnote that the values were read off published
curves and that damping data should come from the supplier of the material;
three of its cells are corrupted in the printing, are registered in this
project's errata and are left empty here rather than guessed at.

Each value is the number its page prints, unless a word in brackets after it says what else it is:

- **converted**: converted from the page's figure

A note mark after a name or a value points to the note the page makes about that row or cell, listed under the table.

| Material | Maximum loss factor | Peak at 10 Hz (°C) | Peak at 100 Hz (°C) | Peak at 1 kHz (°C) | Young's modulus, soft end (MPa) | Young's modulus, stiff end (GPa) | Young's modulus, transition (MPa) | Maximum loss modulus (MPa) | Source |
| --- | --- | --- | --- | --- | --- | --- | --- | --- | --- |
| Antiphon-13 | 1.8 | -3.889 (converted from 25 °F) | 23.89 (converted from 75 °F) | 48.89 (converted from 120 °F) | 8.274 (converted from 1.2e3 psi) | 2.068 (converted from 3e5 psi) | 131 (converted from 1.9e4 psi) | [^damping-1] | Vér & Beranek 2e TABLE 14.1, PDF page 599 (printed p. 598) |
| blachford Aquaplas | 0.5 | 10 (converted from 50 °F) | 26.67 (converted from 80 °F) | 51.67 (converted from 125 °F) | 206.8 (converted from 3e4 psi) | 11.03 (converted from 1.6e6 psi) | 1 517 (converted from 2.2e5 psi) | 758.4 (converted from 1.1e5 psi) | Vér & Beranek 2e TABLE 14.1, PDF page 599 (printed p. 598) |
| Barry Controls H-326 | 0.8 | -40 (converted from −40 °F) | -31.67 (converted from −25 °F) | -23.33 (converted from −10 °F) | 20.68 (converted from 3e3 psi) | 4.137 (converted from 6e5 psi) | 289.6 (converted from 4.2e4 psi) | 234.4 (converted from 3.4e4 psi) | Vér & Beranek 2e TABLE 14.1, PDF page 599 (printed p. 598) |
| Dow Corning Sylgard 188 | 0.6 | 15.56 (converted from 60 °F) | 26.67 (converted from 80 °F) | 43.33 (converted from 110 °F) | 2.068 (converted from 3e2 psi) | 0.1517 (converted from 2.2e4 psi) | 17.93 (converted from 2.6e3 psi) | 10.34 (converted from 1.5e3 psi) | Vér & Beranek 2e TABLE 14.1, PDF page 599 (printed p. 598) |
| EAR C-1002 | 1.9 | -5 (converted from 23 °F) | 12.78 (converted from 55 °F) | 32.22 (converted from 90 °F) | 1.379 (converted from 2e2 psi) | 2.068 (converted from 3e5 psi) | 53.09 (converted from 7.7e3 psi) | 103.4 (converted from 1.5e4 psi) | Vér & Beranek 2e TABLE 14.1, PDF page 599 (printed p. 598) |
| EAR C-2003 | 1 | 7.222 (converted from 45 °F) | 21.11 (converted from 70 °F) | 37.78 (converted from 100 °F) | 4.137 (converted from 6e2 psi) | 5.516 (converted from 8e5 psi) | 151.7 (converted from 2.2e4 psi) | 151.7 (converted from 2.2e4 psi) | Vér & Beranek 2e TABLE 14.1, PDF page 599 (printed p. 598) |
| lord LD-400 | 0.7 | 10 (converted from 50 °F) | 26.67 (converted from 80 °F) | 51.67 (converted from 125 °F) | 22.75 (converted from 3.3e3 psi) | 20.68 (converted from 3e6 psi) | 689.5 (converted from 1e5 psi) | 482.6 (converted from 7e4 psi) | Vér & Beranek 2e TABLE 14.1, PDF page 599 (printed p. 598) |
| Soundcoat DYAD 601 | 1 | -9.444 (converted from 15 °F) | 10 (converted from 50 °F) | 23.89 (converted from 75 °F) | 1.034 (converted from 1.5e2 psi) | 2.068 (converted from 3e5 psi) | 46.19 (converted from 6.7e3 psi) | 46.19 (converted from 6.7e3 psi) | Vér & Beranek 2e TABLE 14.1, PDF page 599 (printed p. 598) |
| Soundcoat DYAD 606 | 1 | 21.11 (converted from 70 °F) | 37.78 (converted from 100 °F) | 54.44 (converted from 130 °F) | 0.8274 (converted from 1.2e2 psi) | [^damping-2] | 41.37 (converted from 6e3 psi) | 41.37 (converted from 6e3 psi) | Vér & Beranek 2e TABLE 14.1, PDF page 599 (printed p. 598) |
| Soundcoat DYAD 609 | 1 | 51.67 (converted from 125 °F) | 65.56 (converted from 150 °F) | 85 (converted from 185 °F) | 4.137 (converted from 6e2 psi) | 1.379 (converted from 2e5 psi) | 75.84 (converted from 1.1e4 psi) | 75.84 (converted from 1.1e4 psi) | Vér & Beranek 2e TABLE 14.1, PDF page 599 (printed p. 598) |
| Soundcoat N | 1.5 | -9.444 (converted from 15 °F) | -1.111 (converted from 30 °F) | 21.11 (converted from 70 °F) | 0.4826 (converted from 7e1 psi) | 2.068 (converted from 3e5 psi) | 31.72 (converted from 4.6e3 psi) | 47.57 (converted from 6.9e3 psi) | Vér & Beranek 2e TABLE 14.1, PDF page 599 (printed p. 598) |
| 3M ISD-110 | 1.7 | 26.67 (converted from 80 °F) | 46.11 (converted from 115 °F) | 65.56 (converted from 150 °F) | 0.2068 (converted from 3e1 psi) | 0.2068 (converted from 3e4 psi) | 6.895 (converted from 1e3 psi) | 11.72 (converted from 1.7e3 psi) | Vér & Beranek 2e TABLE 14.1, PDF page 599 (printed p. 598) |
| 3M ISD-112 | 1.2 | -12.22 (converted from 10 °F) | 4.444 (converted from 40 °F) | 26.67 (converted from 80 °F) | 0.5516 (converted from 8e1 psi) | 0.8963 (converted from 1.3e5 psi) | 22.06 (converted from 3.2e3 psi) | 26.89 (converted from 3.9e3 psi) | Vér & Beranek 2e TABLE 14.1, PDF page 599 (printed p. 598) |
| 3M ISD-113[^damping-3] | 1.1 | -42.78 (converted from −45 °F) | -28.89 (converted from −20 °F) | -9.444 (converted from 15 °F) | 2.068 (converted from 3e2 psi) | 1.034 (converted from 1.5e5 psi) | 1.448 (converted from 2.1e2 psi) | 1.586 (converted from 2.3e2 psi) | Vér & Beranek 2e TABLE 14.1, PDF page 599 (printed p. 598) |
| 3m 468 | 0.8 | -9.444 (converted from 15 °F) | 10 (converted from 50 °F) | 29.44 (converted from 85 °F) | 0.2068 (converted from 3e1 psi) | 0.9653 (converted from 1.4e5 psi) | 13.79 (converted from 2e3 psi) | 11.03 (converted from 1.6e3 psi) | Vér & Beranek 2e TABLE 14.1, PDF page 599 (printed p. 598) |
| 3M ISD-830 | 1 | -59.44 (converted from −75 °F) | -45.56 (converted from −50 °F) | -28.89 (converted from −20 °F) | 1.034 (converted from 1.5e2 psi) | 1.379 (converted from 2e5 psi) | 37.92 (converted from 5.5e3 psi) | 37.92 (converted from 5.5e3 psi) | Vér & Beranek 2e TABLE 14.1, PDF page 599 (printed p. 598) |
| GE SMRD | 0.9 | 10 (converted from 50 °F) | 26.67 (converted from 80 °F) | 51.67 (converted from 125 °F) | 34.47 (converted from 5e3 psi) | [^damping-4] | 268.9 (converted from 3.9e4 psi) | 241.3 (converted from 3.5e4 psi) | Vér & Beranek 2e TABLE 14.1, PDF page 599 (printed p. 598) |

[^damping-1]: the page prints "3.e3e" here, which is not a number in the table's own e-notation, and the defect is registered in docs/ERRATA.md under "Vér & Beranek 2e (2006), TABLE 14.1"
[^damping-2]: the page prints "3G5" here, which is not a number in the table's own e-notation, and the defect is registered in docs/ERRATA.md under "Vér & Beranek 2e (2006), TABLE 14.1"
[^damping-3]: The page prints E_trans = 2.1e2 psi below E_min = 3e2 psi for this row, and footnote c of the same table defines E_min as the smallest value of E. The two cells therefore contradict each other, and the page does not say which of them is wrong: E_I,max = 2.3e2 psi agrees with the printed E_trans through the chapter's own E_I,max = eta_max E_trans, while every other row of the table puts E_trans between one and two orders of magnitude above E_min. Both are served as printed and the defect is registered in docs/ERRATA.md under "Ver & Beranek 2e (2006), TABLE 14.1".
[^damping-4]: the page prints "e35" here, which is not a number in the table's own e-notation, and the defect is registered in docs/ERRATA.md under "Vér & Beranek 2e (2006), TABLE 14.1"

## References

- **Vér, I. L., & Beranek, L. L. (2006).** *Noise and vibration control engineering: Principles and applications* (2nd ed.). Wiley. https://doi.org/10.1002/9780470172568
  Table 14.1: the source of the rows of the catalogue of damping materials that cite it.